Tensile Modulus
Tensile Strength
Charpy impact strength
Description

AKROMIDĀ®

Preliminary

T9 GF 30 grey (8134)

PPA GF30

AKROMIDĀ® T9 GF 30 grey (8134) - PPA, 50% glass fiber, high stiffness and strength, high temperature and chemical resistance, grey RAL 7047, E&E.


Modulus

10.000MPa

Strength

190MPa

Impact

70kJ/mĀ²

AKROMIDĀ® T9 GF 30 grey (8134) - PPA, 50% glass fiber, high stiffness and strength, high temperature and chemical resistance, grey RAL 7047, E&E.

AKROMIDĀ®

C3 1 S3 black (4297)

PA66+PA6

AKROMIDĀ® C3 1 S3 black (4297) - PA 6.6/6 blend unreinforced, impact modified whilst maintaining good flowability, for connecting and fixing systems


Modulus

2.500MPa

Strength

65MPa

Impact

180kJ/mĀ²

AKROMIDĀ® C3 1 S3 black (4297) - PA 6.6/6 blend unreinforced, impact modified whilst maintaining good flowability, for connecting and fixing systems

AKROMIDĀ®

A3 GF 15 1 GIT black (4620)

PA66 GF15

AKROMIDĀ® A3 GF 15 1 GIT black (4620) - 15% Glasfaser, heat stabilised, easy flowing polyamide 6.6, gas injection technology, excellent surface


Modulus

5.500MPa

Strength

125MPa

Impact

40kJ/mĀ²

AKROMIDĀ® A3 GF 15 1 GIT black (4620) - 15% Glasfaser, heat stabilised, easy flowing polyamide 6.6, gas injection technology, excellent surface

AKROMIDĀ®

Preliminary

B3 GM 10/20 1 black (8748)

PA6 (GF10+GB20)

AKROMIDĀ® B3 GM 10/20 1 black (8748) - PA6, 10% glass fibre, 20% glass bead, heat stabilised, easy flowing, good surface, reduced warpage.


Modulus

5.700MPa

Strength

110MPa

Impact

30kJ/mĀ²

AKROMIDĀ® B3 GM 10/20 1 black (8748) - PA6, 10% glass fibre, 20% glass bead, heat stabilised, easy flowing, good surface, reduced warpage.

AKROMIDĀ®

B3 GF 50 1 grey (5507)

PA6 GF50

AKROMIDĀ® B3 GF 50 1 grey (5507) - 50% glass fiber reinforced PA 6, heat stabilised, technical parts in industrial engineering and automotive industry


Modulus

16.500MPa

Strength

190MPa

Impact

70kJ/mĀ²

AKROMIDĀ® B3 GF 50 1 grey (5507) - 50% glass fiber reinforced PA 6, heat stabilised, technical parts in industrial engineering and automotive industry

AKROTEKĀ®

PK-VM CF 10 TM black (6135)

PK CF10

AKROTEKĀ® PK-VM CF 10 TM black (6135) - Polyketon, 10% carbon fiber reinforced, chemical, tribological modification, high elongation at break


Modulus

3.500MPa

Strength

59MPa

Impact

100kJ/mĀ²

AKROTEKĀ® PK-VM CF 10 TM black (6135) - Polyketon, 10% carbon fiber reinforced, chemical, tribological modification, high elongation at break

AKROMIDĀ®

A3 ICF 30 5 black (6495)

PA66 CF30

AKROMIDĀ® A3 ICF 30 5 black (6495) is a 30% carbon fibre reinforced, high heat stabilised polyamide 6.6 with high flexural strength and good sliding properties


Modulus

23.000MPa

Strength

235MPa

Impact

50kJ/mĀ²

AKROMIDĀ® A3 ICF 30 5 black (6495) is a 30% carbon fibre reinforced, high heat stabilised polyamide 6.6 with high flexural strength and good sliding properties

143444580

AKROMIDĀ®

A3 GM 20/10 S1 black (4817)PA66-I (GF20+GB10)

AKROMIDĀ® A3 GM 20/10 S1 black (4817) is a 20% glass fiber and 10% glass beads reinforced, impact modified PA 6.6. It is characterised by a medium cold impact strength as well as a good surface appearance and low warpage. It is therefore perfectly suitable for technical demanding components in the mechanical engineering and automotive industry.

Features

impact modified
surface modified
low warpage

Properties

Modulus

6.900MPa

Strength

130MPa

Impact

80kJ/mĀ²

Mechanical Properties


Tensile modulus

ISO 527-2

1 mm/min | d.a.m.
1 mm/min | conditioned
6900 MPa
4200 MPa

Tensile stress at break

ISO 527-2

5 mm/min | d.a.m.
5 mm/min | conditioned
130 MPa
85 MPa

Tensile strain at break

ISO 527-2

5 mm/min | d.a.m.
5 mm/min | conditioned
4 %
10 %

Flexural modulus

ISO 178

2 mm/min | d.a.m.
6900 MPa

Flexural strength

ISO 178

2 mm/min | d.a.m.
205 MPa

Charpy impact strength

ISO 179-1/1eU

23Ā°C | d.a.m.
23Ā°C | conditioned
30Ā°C | d.a.m.
-
80 kJ/mĀ²
80 kJ/mĀ²
76 kJ/mĀ²

Charpy notched impact strength

ISO 179-1/1eA

23Ā°C | d.a.m.
23Ā°C | conditioned
30Ā°C | d.a.m.
-
15 kJ/mĀ²
16 kJ/mĀ²
8 kJ/mĀ²

Ball indentation hardness

ISO 2039-1

358N/30s | d.a.m.
127 MPa

Thermal Properties


Temperature of deflection under load HDT/A

ISO 75

1,8 MPa
245 Ā°C

Temperature of deflection under load HDT/B

ISO 75

0,45 MPa
260 Ā°C

Melting temperature

ISO 11357-3

DSC, 10K/min
262 Ā°C

Coefficient of linear thermal expansion

ISO 11359-1/2

23Ā°C to 80Ā°C | parallel
23Ā°C to 80Ā°C | transverse
0,27 10ā»ā“/K
1,11 10ā»ā“/K

Flammability


Burning rate

UL 94

1,6 mm Wall thickness
HB Class

Burning rate (<100 mm/min)

FMVSS 302

> 1 mm Thickness
+

General properties


Density

ISO 1183

23Ā°C
1,31 g/cmĀ³

Humidity absorption

ISO 1110

70Ā°C, 62% r.H.
2 %

Water absorption

ISO 62

23Ā°C, saturated
5,1 %

Molding shrinkage

ISO 294-4

flow
transverse
0,5 %
1,3 %

Disclaimer

All specifications and information given on this website are based on our current knowledge and experience. A legally binding promise of certain characteristics or suitability for a concrete individual case cannot be derived from this information. The information supplied here is not intended to release processors and users from the responsibility of carrying out their own tests and inspections in each concrete individual case. AKROĀ®, AKROMIDĀ®, AKROLENĀ®, AKROLOYĀ®, AKROTEKĀ®, ICXĀ® and PRECITEĀ® are registered trademarks of the Feddersen Group.

Contact

Do you have any questions? We are happy to help.

Would you like to learn more about AKRO-PLASTIC GmbH? Contact us! We will be happy to help you.

Learn more