HEADER Granulat 1920x700

Find the right compound

Select your fitting and find the right compound for your intend

Tensile Modulusin MPa
Tensile Strengthin MPa
Charpy impact strengthin kJ/mĀ²
558 Compounds found
Recommended Ā 
Tensile Modulus
Tensile Strength
Charpy impact strength
Description

AKROTEKĀ®

Preliminary

PPS GF 40 black (8609)

PPS GF40

AKROTEKĀ® PPS GF 40 black (8609) is a 40% glass fibre reinforced Polyphenylene sulfide with high rigidity and strength, as well as high temperature and chemical resistance.


Modulus

16.000MPa

Strength

180MPa

Impact

50kJ/mĀ²

AKROTEKĀ® PPS GF 40 black (8609) is a 40% glass fibre reinforced Polyphenylene sulfide with high rigidity and strength, as well as high temperature and chemical resistance.

AKROTEKĀ®

Preliminary

PK-VM GF 15 natural (8680)

PK GF15

AKROTEKĀ® PK-VM GF 15 natural (8680) - Polyketon, 15% glass fiber reinforced, chemical and hydrolysis resistance


Modulus

4.600MPa

Strength

100MPa

Impact

65kJ/mĀ²

AKROTEKĀ® PK-VM GF 15 natural (8680) - Polyketon, 15% glass fiber reinforced, chemical and hydrolysis resistance

AKROMIDĀ®

UL

B3 GF 35 1 HU red (8416)

PA6 GF35

AKROMIDĀ® B3 GF 35 1 HU red (8416) - PA 6, 35% glass fibre, heat ageing resistant, high rigidity and strength, UL listed HB.


Modulus

12.000MPa

Strength

190MPa

Impact

NA

AKROMIDĀ® B3 GF 35 1 HU red (8416) - PA 6, 35% glass fibre, heat ageing resistant, high rigidity and strength, UL listed HB.

AKROTEKĀ®

Preliminary

PPS GF 40 natural (8064)

PPS GF40

AKROTEKĀ® PPS GF 40 natural (8064) is a 40% glass fibre reinforced Polyphenylene sulfide with high rigidity and strength, as well as high temperature and chemical resistance.


Modulus

12.000MPa

Strength

190MPa

Impact

50kJ/mĀ²

AKROTEKĀ® PPS GF 40 natural (8064) is a 40% glass fibre reinforced Polyphenylene sulfide with high rigidity and strength, as well as high temperature and chemical resistance.

AKROTEKĀ®

Preliminary

PK-VM GF 40 black (8687)

PK GF40

AKROTEKĀ® PK-VM GF 40 black (8687) - Polyketon, 40% glass fibre reinforced, chemical restistant


Modulus

11.000MPa

Strength

160MPa

Impact

80kJ/mĀ²

AKROTEKĀ® PK-VM GF 40 black (8687) - Polyketon, 40% glass fibre reinforced, chemical restistant

AKROTEKĀ®

Preliminary

AM ICF 20 black (8722)

ABSCF20

AKROTEKĀ® AM ICF 20 black (8722) - recycled carbon fibre reinforced for additive manufacturing (3D-printing)


Modulus

13.400MPa

Strength

100MPa

Impact

20kJ/mĀ²

AKROTEKĀ® AM ICF 20 black (8722) - recycled carbon fibre reinforced for additive manufacturing (3D-printing)

AKROMIDĀ®

B28 GF 30 S3 black (8438)

PA6-I GF30

AKROMIDĀ® B28 GF 30 S3 black (8438) - PA 6, 30% glass fiber reinforced, impact modified, industrial applications, housings and covers, automotive


Modulus

9.000MPa

Strength

155MPa

Impact

100kJ/mĀ²

AKROMIDĀ® B28 GF 30 S3 black (8438) - PA 6, 30% glass fiber reinforced, impact modified, industrial applications, housings and covers, automotive

175767780

AKROMIDĀ®

A3 GF 30 3 black (21005)PA66 GF30

AKROMIDĀ® A3 GF 30 3 black (21005) is a 30% glass fiber reinforced polyamide 6.6. It is characterised by high stiffness and strength. Furthermore, the material is nucleated and anorganic heat stabilised and therefore perfectly suitable for technical parts in industrial engineering and in the automotive industry which are exposed to higher temperatures.

Features

heat stabilised 160
nucleated

Properties

Modulus

10.000MPa

Strength

170MPa

Impact

55kJ/mĀ²

Mechanical Properties


Tensile modulus

ISO 527-2

1 mm/min | d.a.m.
1 mm/min | conditioned
10000 MPa
7000 MPa

Tensile stress at break

ISO 527-2

5 mm/min | d.a.m.
5 mm/min | conditioned
170 MPa
100 MPa

Tensile strain at break

ISO 527-2

5 mm/min | d.a.m.
5 mm/min | conditioned
2,5 %
5 %

Flexural modulus

ISO 178

2 mm/min | d.a.m.
8800 MPa

Charpy impact strength

ISO 179-1/1eU

23Ā°C | d.a.m.
23Ā°C | conditioned
55 kJ/mĀ²
65 kJ/mĀ²

Charpy notched impact strength

ISO 179-1/1eA

23Ā°C | d.a.m.
23Ā°C | conditioned
8 kJ/mĀ²
11 kJ/mĀ²

Thermal Properties


Temperature of deflection under load HDT/A

ISO 75

1,8 MPa
255 Ā°C

Temperature of deflection under load HDT/B

ISO 75

0,45 MPa
260 Ā°C

Melting temperature

ISO 11357-3

DSC, 10K/min
262 Ā°C

Vicat softening temperature B50

ISO 306

50Ā°C/50N
> 230 Ā°C

Flammability


Burning rate

UL 94

1,6 mm Wall thickness
HB Class

Burning rate (<100 mm/min)

FMVSS 302

> 1 mm Thickness
+

General properties


Density

ISO 1183

23Ā°C
1,37 g/cmĀ³

Humidity absorption

ISO 1110

70Ā°C, 62% r.H.
1,9 - 2,1 %

Molding shrinkage

ISO 294-4

flow
transverse
0,1 - 0,3 %
0,7 - 0,9 %

Disclaimer

All specifications and information given on this website are based on our current knowledge and experience. A legally binding promise of certain characteristics or suitability for a concrete individual case cannot be derived from this information. The information supplied here is not intended to release processors and users from the responsibility of carrying out their own tests and inspections in each concrete individual case. AKROĀ®, AKROMIDĀ®, AKROLENĀ®, AKROLOYĀ®, AKROTEKĀ®, ICXĀ® and PRECITEĀ® are registered trademarks of the Feddersen Group.

Contact

Do you have any questions? We are happy to help.

Would you like to learn more about AKRO-PLASTIC GmbH? Contact us! We will be happy to help you.

Learn more